Average Density of Amorphous Polymers

Amorphous Polymer  ρam1
(g/cm3)
Poly(vinyl chloride), PVC 1.388
Poly(vinyl fluoride), PVF 1.340
Poly(vinylidene fluoride), PVDF 1.675
Polychloroprene, Neoprene 1.243
Poly(2-cyanoethyl acrylate) 1.403
Poly(acrylic acid), PAA 1.410
Poly(butyl acrylate) , PBA 1.080
Poly(methyl acrylate), PMA 1.224
PoIy(1-hexene) 0.865
Poly(1-butene), PB-1 0.860
Poly(4-methyl-1-pentene) 0.836
Poly(ethylene), PE 0.854
Poly(isobutene) 0.864
Poly(propylene), PP 0.861
Poly(8-aminooctanoic acid), Nylon 8 1.039
Poly(caprolactam) 1.084
Poly(hexamethylene adipamide), Nylon6,6 1.078
Poly(hexamethylene dodecanediamide), Nylon 6,12 1.070
Poly(m-phenylene terephthalamide), Nomex MPDI 1.355
Poly(p-phenylene terephthalamide) (spun), Kevlar, PPTA 1.439
Poly(ω-dodecanamide), Nylon 12 1.000
Poly(ω-undecanamide), Nylon 11 1.018
Poly(Bisphenol A carbonate), PC 1.206
Poly(methyl cyanoacrylate) 1.327
PoIy(1,2-butadiene) 0.912
Poly(1,4-butadiene), PBD 0.891
Poly(caprolactone), PCL 1.120
Poly(cyclohexylenedimethylene terephthalate) 1.195
Poly(decamethylene terephthalate) 1.017
Poly(ethylene adipate) 1.205
Poly(ethylene terephthalate), PET 1.333
Poly(trimethylene terephthalate) 1.340
Poly[(tetramethylene terephthalate), PBT 1.310
Polyglycolide, PGA, PGL 1.523
Polylactic acid, PLA 1.248
Poly(ether ketone ketone), PEKK 1.279
Poly[(ether ether ketone) PEEK 1.264
Poly(epichlorohydrin) 1.344
Poly(ethylene glycol), PEO, PEG 1.128
Poly(propylene glycol), PPG 1.004
Poly(tetrahydrofuran), PTMO, PTHF 0.978
Polyacetal, Poly(methylene oxide), POM 1.225
Poly(benzyl methacrylate) 1.173
Poly(butyl methacrylate), PBMA 1.053
Poly(cyclohexyl methacrylate), PCHMA 1.100
Poly(ethyl methacrylate), PEMA 1.117
Poly(hexyl methacrylate), PHMA 1.008
Poly(isobutyl methacrylate), PIBMA 1.053
Poly(isopropyl methacrylate), PIPMA 1.053
Poly(methyl methacrylate), PMMA 1.159
Poly(phenyl methacrylate) 1.211
Poly(propyl methacrylate), PPMA 1.077
Poly(tert-butyl methacrylate) 1.023
Poly(acrylonitrile), PAN 1.184
Poly(methacrylonitrile) 1.115
Poly(p-phenylene), PPP 1.110
Poly(p-xylene) 1.050
Poly(2,6-dimethyl-p-phenylene oxide), PPO, PPE 1.058
Poly(2-methylstyrene) 1.029
Poly(4-methylstyrene), PMS, PPMS 1.027
Poly(4-tert-butylstyrene) 0.950
Poly(α-methylstyrene), PAMS 1.070
Polystyrene, PS 1.052
Poly(1,4-biphenyl ether ether sulfone), PPSU 1.290
Poly(1,4-phenylene ether-sulfone), PES 1.370
Poly{[bis(4-chlorophenyl)sulfone]-alt-[bisphenol-A]}, PSU 1.235
Poly(thio-1,4-phenylene), PPS 1.350
Poly(propylene sulfide), PPS 1.082
Poly(vinyl alcohol), PVOH 1.300
Poly(vinyl acetate), PVA, PVAC 1.190
Poly(vinyl butyrate), PVB 1.093
Poly(vinyl propionate) 1.117
Poly(butyl vinyl ether) 0.919
Poly(ethyl vinyl ether) 0.954
Poly(isobutyl vinyl ether) 0.915
Poly(methyl vinyl ether), PVME 1.044
Poly(propyl vinyl ether) 0.981
Poly(methyl isopropenyl ketone) 1.135
Poly(vinyl ethyl ketone) 1.028
Poly(vinyl methyl ketone) 1.120
Poly(methyl vinyl thioether) 1.110
Poly(vinyl phenyl sulfide) 1.153
 
1 The densities are the average of one or more experimental values.

  •